Properties List
Properties Table List
Standard Grade
| Item | Test condition |
Test Method |
Units | XN400 | XG310A30A | XG310A50A | XG510A30D | XG510A50D | |
|---|---|---|---|---|---|---|---|---|---|
| Non- reinforced |
GF reinforced Good flow |
GF reinforced Good flow |
GF reinforced |
GF reinforced |
|||||
| Mechanical Properties |
Tensile stress | At yield | ISO 527-1, -2 | MPa | 84 | 144 | 190 | 181 | 223 |
| Tensile strain | At break | ISO 527-1, -2 | % | 7 | 4 | 4 | 5 | 5 | |
| Flexural strength | — | ISO 178 | MPa | 110 | 238 | 310 | 264 | 344 | |
| Flexural modulus | — | ISO 178 | MPa | 2500 | 8300 | 15000 | 8900 | 14800 | |
| Charpy impact strength |
With notch | ISO 179-1eA | kJ/m² | 5 | 8 | 10 | 10 | 13 | |
| Rockwell hardness | R scale | ISO 2039 | — | — | 120 | 120 | 120 | 120 | |
| Thermal Properties |
DTUL | 1.8MPa | ISO 75-1, -2 | °C | 123 | 302 | 308 | 302 | 310 |
| Electronic Properties |
Dielectric constant | 1MHz | IEC 60250 | — | — | 3.8 | — | — | — |
| Comparative tracking Index |
— | IEC 60112 | V | — | 600 | — | — | — | |
| Flow Properties |
MFR | Load 1.2kg | ISO 1133 | g/10min | 30 | 30 | 25 | 7 | 5 |
| °C | 330 | 340 | 340 | 340 | 340 | ||||
| Other Properties |
Density | — | ISO 1183 | g/cm³ | 1.14 | 1.36 | 1.57 | 1.36 | 1.57 |
| Mold shrinkage | MD | ISO 294-4 | % | 1.5 | 0.2 | 0.2 | 0.2 | 0.2 | |
| TD | 1.5 | 0.6 | 0.5 | 0.6 | 0.5 | ||||
Last Updated: 12 February 2015
High function grade
| Item | Test condition |
Test Method |
Units | XV310A30 | XI500 | XD361A40 | XB510A30D | |
|---|---|---|---|---|---|---|---|---|
| Flame- resistant |
High Toughness |
Precision molding |
CF reinforced |
|||||
| Mechanical Properties |
Tensile stress | At yield | ISO 527-1, -2 | MPa | 150 | 49 | 99 | 227 |
| Tensile strain | At break | ISO 527-1, -2 | % | 4 | 32 | 3 | 4 | |
| Flexural strength | — | ISO 178 | MPa | 220 | 69 | 165 | 336 | |
| Flexural modulus | — | ISO 178 | MPa | 11500 | 1600 | 9700 | 19200 | |
| Charpy impact strength |
With notch | ISO 179-1eA | kJ/m² | 10 | 84 | 2 | 7 | |
| Rockwell hardness | R scale | ISO 2039 | — | — | — | — | — | |
| Thermal Properties |
DTUL | 1.8MPa | ISO 75-1, -2 | °C | 302 | 112 | 278 | 302 |
| Electronic Properties |
Dielectric constant | 1MHz | IEC 60250 | — | 3.7 | — | — | — |
| Comparative tracking Index |
— | IEC 60112 | V | 425 | — | — | — | |
| Flow Properties |
MFR | Load 1.2kg | ISO 1133 | g/10min | 10 | — | 25 | 9 |
| °C | 340 | — | 330 | 340 | ||||
| Flammability | — | — | UL94 | V-0 | ||||
| Other Properties |
Density | — | ISO 1183 | g/cm³ | 1.60 | 1.07 | 1.49 | 1.28 |
| Mold shrinkage | MD | ISO 294-4 | % | 0.2 | 1.4 | 0.4 | 0.2 | |
| TD | 0.4 | 1.4 | 0.5 | 0.6 | ||||
Last Updated: 12 February 2015
LED Reflectors
| Item | Test condition |
Test Method |
Units | XR300A37 | XR310A45 | |
|---|---|---|---|---|---|---|
| High-gloss | Standard | |||||
| Mechanical Properties |
Tensile stress | At yield | ISO 527-1, -2 | MPa | 50 | 95 |
| Tensile strain | At break | ISO 527-1, -2 | % | 2 | 4 | |
| Flexural strength | — | ISO 178 | MPa | 92 | 150 | |
| Flexural modulus | — | ISO 178 | MPa | 3700 | 6300 | |
| Charpy impact strength |
With notch | ISO 179-1eA | kJ/m² | 2 | 2 | |
| Rockwell hardness | R scale | ISO 2039 | — | — | — | |
| Thermal Properties |
DTUL | 0.45MPa | ISO 75-1, -2 | °C | 256 | 304 |
| Electronic Properties |
Dielectric constant | 1MHz | IEC 60250 | — | — | — |
| Comparative tracking Index |
— | IEC 60112 | V | — | — | |
| Flow Properties |
MFR | Load 1.2kg | ISO 1133 | g/10min | — | — |
| °C | — | — | ||||
| Other Properties |
Density | — | ISO 1183 | g/cm³ | 1.53 | 1.59 |
| Mold shrinkage | MD | ISO 294-4 | % | 0.7 | 0.4 | |
| TD | 1.2 | 0.5 | ||||
Last Updated: 12 February 2015